Cold-rolled steel for forming has the following mechanical properties (skin-passed) - these are measured transverse to the rolling direction:
|
EN 10130, 2006
|
Re max.1 2 3 6)
|
Rm min.-max.
|
A80
|
r90
|
n90
|
|
Grade
|
N/mm²
|
N/mm²
|
Min.2 3) %
|
Min.4 5)
|
Min.4)
|
|
DC01
|
280
|
270-410
|
28
|
-
|
-
|
|
DC03
|
240
|
270-370
|
34
|
1.3
|
-
|
|
DC04
|
210
|
270-350
|
38
|
1.6
|
0.180
|
|
DC05
|
180
|
270-330
|
40
|
1.9
|
0.200
|
|
DC06
|
170
|
270-330
|
41
|
2.1
|
0.220
|
1) The values of the yield strength are those of the 0.2% yield strength for products with no definite yield point
and the lower yield strength ReL for the other products. 2) For a thickness of 0.5 mm < t ≤ 0.7 mm the maximum value of the yield strength is increased by 20 N/mm²
and the minimum elongation after fracture is decreased by 2%. 3) For a thickness of t ≤ 0.5 mm the maximum value of the yield strength is increased by 40 N/mm²
and the minimum elongation after fracture is decreased by 4%. 4) The r and n values apply to a thickness of t ≥ 0.5 mm. 5) For a thickness of t > 2 mm, the r90 value or rav value is decreased by 0.2. 6) For design purposes, a lower yield strength ReL of at least 120 N/mm² can be assumed. |